Specific application of polyurethane catalysts in several typical polyurethane flexible foams

1. Typical formula and performance of block polyether type PU soft foam

Polyether Triol 100pbw

TDI80/20 46.0pbw

Organotin catalyst 0.4pbw

Tertiary amine catalyst 0.2pbw

Silicone Foam Stabilizer 1.0pbw

Water 3.6pbw

Foaming aid 0~12pbw

Performance:

Foam density, kg/m3 22.4

Tensile strength, kpa 96.3

Elongation, % 220

Tear strength, N/m 385

Compression set, 50% 6

90% 6

Cave load, kg

(38cm×35.6cm×10cm)

Transformation 25% 13.6

65% 25.6

Falling ball rebound, % 38

In recent years, in order to meet the needs of the market, some enterprises often produce foams with low density (10kg/m3). In addition, there must be a relatively high stability silicon surfactant and catalyst.

Reference formula for producing low-density ultra-low-density soft foam:

name Medium Density Low density Super low density
Continuous box style Continuous box style box style
Polyether polyol 100 100 100 100 100
Water 3.0 3.0 4.5 Tensile strength, kPa 124

Spring rate, % ≥ 60

Compression deformation, 75% ≤8

Oxygen index, OI% ≥ 28

Smoke Density ≤50

9. Water is the foaming agent, fully environmentally friendly Self-skin foam

HCFC-141b blowing agent has been completely banned in foreign countries. CP blowing agents are flammable. HFC-245fa and HFC-365mfc blowing agents are expensive and unacceptable. The only way out is to use water as a blowing agent to synthesize environmentally friendly self-bonding skin foam. In the past, PU workers at home and abroad only paid attention to the modification of polyether and isocyanate, so the surface layer of the produced foam was unclear and dense.

A set of formulas is recommended, which features:

  • The basic polyether polyol remains unchanged, and the conventional Mn5000 or 6000 is used. ·

  • The isocyanate remains unchanged, and C-MDI, PAPI or modified MDI can be used.

  • It can be solved by using special additive SH-140. ·

Basic recipe:

  • Highly active polyether triol Mn5000 65pbw

  • SH-140* 35pbw

  • Chain Extender: 1,4-Butanediol 5pbw

  • Cross-linking agent: glycerin 7pbw

  • Cell opener: K-6530 0.2~0.5pbw

  • Catalyst A-2 1.2~1.3pbw

  • Proper amount of color paste

  • Water 5pbw

  • MR-200 45pbw

Note: *SH-140 is our product.

Physical properties:

Overall foam density 340~350kg/m3

Products: Smooth surface, clear crust, low density.

px; margin: 0px; padding-left: 0px; padding-right: 0px; font: 12px/24px Arial, Verdana, sans-serif; white-space: normal; letter-spacing: normal; color: rgb(51 ,51,51); word-spacing: 0px; padding-top: 10px; -webkit-text-stroke-width: 0px”>
Basic recipe:

  • Highly active polyether triol Mn5000 65pbw

  • SH-140* 35pbw

  • Chain Extender: 1,4-Butanediol 5pbw

  • Cross-linking agent: glycerin 7pbw

  • Cell opener: K-6530 0.2~0.5pbw

  • Catalyst A-2 1.2~1.3pbw

  • Proper amount of color paste

  • Water 5pbw

  • MR-200 45pbw

Note: *SH-140 is our product.

Physical properties:

Overall foam density 340~350kg/m3

Products: Smooth surface, clear crust, low density.

Call Us

+86-189 6236 5658

Email: edisonzhao@51qiguang.com

Working hours: Monday to Friday, 9:00-17:30 (GMT+8), closed on holidays
Scan to open our site